A smooth weld surface does not tell you much about what is underneath it. A seam can look consistent under a microscope and still contain internal pores. The problem may only become visible after sectioning, during a leak test, or when a joint fails a mechanical test.

Changing laser power is an obvious next step. It is not always the useful one.

Surface contamination, poor shielding coverage, and an unstable keyhole can all contribute to porosity, but they need different corrective actions. TWI identifies these as separate causes of pores in laser welds, including hydrogen-related porosity in aluminum.

For thin metal joints, a practical investigation starts with the failed sample: where the cavities are, what surrounds them, and whether the same pattern appears again. The sequence below is a troubleshooting approach, not a qualified welding procedure.

The images in this article are explanatory illustrations, not production photographs or measured test results.

Keep the failed sample—and its orientation

Before cleaning, polishing, or re-welding a suspect part, photograph it and mark the welding direction. Record the start, stop, fixture position, and sample number.

That information becomes difficult to recover after the part has been cut apart.

On a circular seam, for example, “porosity near the edge” is not a useful description. A pore at the seam closure raises different questions from pores scattered around the circumference.

A simple defect map can guide the next check:

Defect location and initial troubleshooting checks
Observed patternFirst checks worth making
Defects concentrated at the startGas preflow, initial surface condition, power ramp, and motion synchronization
Cavities near the stop or seam closurePower termination, overlap, local reheating, and crater formation
Defects repeating at the same fixture locationFit-up, clamping, beam access, and shielding obstruction
Defects scattered through the seamSurface preparation, material condition, gas delivery, and melt-pool stability

These are starting hypotheses. Location alone does not establish the cause.

Also confirm that the feature is actually a pore. An unbonded interface, a shrinkage cavity, or material pulled out during metallographic preparation can be mistaken for gas porosity. If a dark feature follows the original joint line, investigate fusion before calling it a trapped bubble.

Check the surfaces that disappear inside the joint

For a lap joint, inspecting the exposed top surface is not enough. The two mating surfaces become inaccessible after assembly, and that is where contamination can be missed.

Check the condition of the parts before they enter the fixture:

  • Is machining fluid still present around an edge or locating feature?
  • Does the cleaning process reach both mating surfaces?
  • Are the parts fully dry before assembly?
  • Is there plating, an adhesive residue, or a protective coating in the weld path?
  • Are cleaned parts handled or stored in a way that reintroduces contamination?

“Cleaned before welding” needs to describe a repeatable process. It should include the cleaning method, drying, handling, and time before welding—not just the fact that somebody wiped the part.

The material matters here. TWI describes moisture-bearing surface layers as a hydrogen source in titanium welding, with pores forming during solidification. A visually clean surface is therefore not sufficient evidence that the joint preparation is suitable.

A useful comparison is to hold the welding schedule constant and test a documented surface-preparation change on representative samples. If cleaning, fit-up, and power are all changed together, an improved result will not tell you which change helped.

Inspect shielding at the joint, not just at the flowmeter

A flowmeter confirms a setting upstream. It does not confirm that the molten weld is receiving consistent protection.

Look at the nozzle with the actual component clamped in place. A clamp jaw, a recessed seam, or the component wall itself may interfere with the gas path. An arrangement that works on an open coupon may behave differently inside an assembled housing.

Illustration comparing clear shielding gas access and clamp-obstructed gas access at a thin metal lap joint
Gas access must be checked with the actual fixture in place. Flow arrows are schematic, not CFD or measured gas-flow data.

Record nozzle angle, distance from the joint, gas composition, preflow, and postflow. Check the delivery line for leaks and the nozzle for damage or blockage.

Increasing flow is not automatically an improvement. Excessive flow can create turbulence and draw surrounding air into the shielding region. TWI lists gas-line leaks, excessive flow, drafts, and turbulence among the causes of inadequate protection and porosity.

If a defect repeatedly occurs beside one clamp, changing the entire laser schedule may be a poor first experiment. Check whether the clamp is affecting gas access or part seating.

Gas selection also needs to remain material-specific. Do not transfer a shielding-gas recipe to another alloy simply because the first weld had an attractive surface.

Decide whether the problem is gas generation or gas entrapment

These mechanisms can occur together, but separating them makes the investigation more useful.

Contamination, moisture, and some coatings can supply gas or vapor during welding. Cleaning and material preparation address that source.

Keyhole instability is different. During keyhole welding, a vapor cavity forms within the molten material. If the cavity becomes unstable and closes unfavorably, a void may remain as the surrounding metal solidifies. Cleaner surfaces alone do not necessarily correct that behavior.

First establish the actual welding regime. Do not assume that a small weld is operating in conduction mode, or that every deep cavity is evidence of excessive power. The distinction between conduction and keyhole welding affects which adjustments are worth testing.

Then examine the suspect region together with the fusion profile. A reduced pore count is not a successful correction if the weld no longer reaches the required interface.

Pay attention to how the weld ends

When cavities are concentrated at the end of a pulsed weld or seam, review the power termination separately from the steady welding condition.

The relevant variables may include the pulse tail, power downslope, travel synchronization, or the way the seam closes over its starting region.

Pulse shaping can help in suitable applications. AMADA WELD TECH describes using the later portion of a pulse to control cooling and reduce porosity or cracking in section 6.4 of its Laser Welding Fundamentals. That supports testing a controlled energy withdrawal; it does not provide one universal pulse shape for every joint.

A longer downslope also changes the thermal cycle. Check the result for penetration, weld width, distortion, and any effects on neighboring features.

For an overlapping pulsed seam, inspect between pulse centers as well as through them. A section through the deepest part of one spot may miss insufficient joining between adjacent spots.

Run a trial that leaves an interpretable result

A small, documented comparison is more useful than a collection of samples made under uncertain conditions.

Keep a baseline recipe and retain baseline samples. Number each subsequent trial before welding it.

Start with process checks that do not require a new laser schedule: surface preparation, fixture seating, gas delivery, and actual focal position. Once those are controlled, select parameter changes that address the suspected mechanism.

For each trial, record:

  • Material grade, thickness, condition, and relevant coating information.
  • Joint geometry, measured fit-up, and fixture identification.
  • Laser schedule, focal position, travel conditions, and gas arrangement.
  • Inspection method and the exact region inspected.
  • Both the porosity result and whether the required fusion was retained.

Testing one factor at a time can help isolate an initial cause. Later development may require a structured experiment because power, speed, focus, and pulse shape interact.

Repeat the promising condition. One favorable section is a reason to continue testing, not a reason to release production.

Where the production process warms the fixture or component over successive cycles, include that condition in the evaluation. A cold first sample should not be the only basis for accepting a repeat-production schedule.

Choose inspection around the question

“Inspect for porosity” is incomplete. Specify whether the question concerns internal cavities, fusion geometry, a leak path, or joint performance.

Metallographic sections

A prepared section can show a cavity’s relationship to the fusion boundary, joint interface, and weld root. It is especially useful when investigating whether a parameter change has reduced penetration.

Its limitation is sampling. A section shows one plane. It cannot establish the condition of the entire seam.

Illustration showing section planes A and C intersecting weld pores while section B misses them in thin metal foil
A pore-free section plane does not establish that the entire weld is pore-free. The enlarged longitudinal view is an illustration, not a metallographic test result.

Choose section locations from the defect map. If the concern is seam closure, cutting only through the middle of the steady seam misses the region under investigation.

Radiography and computed tomography

Radiography can reveal internal porosity, but detection depends on the material, geometry, and inspection technique. TWI specifically notes the difficulty of detecting small pores and the influence of the material being examined.

CT adds three-dimensional information, which can help locate cavities and examine their distribution. However, the scan must have suitable detection capability for the defect of concern. A quoted voxel size is not, by itself, a demonstrated minimum detectable pore size. NIST’s description of micro-CT emphasizes imaging features within a particular size range and the importance of sample stability during scanning.

Ask the inspection provider what can be detected in the actual component—not only in a small demonstration sample.

Leak testing

A leak test answers a different question: can gas pass through the component under the specified test conditions?

Tracer-gas methods depend on gas moving through a leak path. An isolated internal pore may not form such a path, so passing a leak test does not establish that the weld contains no internal cavities.

For a sealing joint, leak testing and internal inspection may therefore provide complementary evidence. Neither automatically replaces the other.

Define what “acceptable” means before signing off

There is no useful universal pore limit for all micro-welded parts.

A sealing enclosure, a mechanically loaded bracket, and an electrical connection have different functional requirements. Acceptance needs to follow the drawing, applicable specification, and agreed validation plan.

Even a percentage-porosity result needs context. Is it an area fraction measured on selected sections, or a volume fraction from CT? What region was evaluated? Were the largest cavity and its location recorded? Those results should not be treated as interchangeable.

Avoid reporting only “porosity-free.” A more defensible statement identifies the inspected samples, method, locations, detection capability, and acceptance criteria.

The development record should let another engineer reconstruct the result: which condition failed, what changed, where the revised weld was inspected, and whether fusion and functional performance still met the requirement.

That record is what makes the correction usable on the next batch.